ISO 12945-2 Modified Martindale Pilling Test Guide

2026年09月09日 09時57分40秒

A practical overview of the ISO 12945-2 Modified Martindale approach for assessing textile surface pilling, fuzzing, and matting.

The ISO 12945-2 Martindale pilling test is used to assess a fabric’s tendency to develop surface pilling, fuzzing, or matting during rubbing. These visible changes can affect the appearance of a textile, although the acceptable level may vary with the garment type and intended end use.

The method described in ISO 12945-2:2020 uses the Modified Martindale approach. It subjects specimens to rubbing under controlled conditions and supports a visual comparison of the tested fabric surface. For textile manufacturers, quality-control laboratories, and researchers, the test provides a structured way to examine changes that may occur as a fabric is worn.

ISO 12945-2 Martindale abrasion tester for textile pilling assessment

What the Modified Martindale Method Evaluates

Fabric surfaces can change when fibers migrate from the structure and become entangled through use. The Modified Martindale method focuses on three related surface conditions:

  • Pilling: the formation of small fiber balls on the fabric surface.
  • Fuzzing: the development of a fuzzy surface texture.
  • Matting: the flattening or compaction of fibers, which can change texture and visual appearance.

Because these conditions are assessed on the surface, specimen condition, preparation, rubbing, and grading should be considered as parts of one consistent evaluation process. A clear agreement on specimen condition before the test is especially useful when results are being compared.

Key Conditions Before Testing

Testing is conducted under standard environmental conditions. The method is not applicable to fabrics thicker than 3 mm because the fabric gripper cannot adequately secure those specimens.

Specimens may be assessed before or after washing. Washing or dry-cleaning before testing is recommended in the source procedure, and both treatments may be used where necessary. However, the selected specimen condition should be agreed by the parties involved before testing begins. This helps ensure that the reported result is understood in the context of the fabric’s treatment state.

Specimen Preparation for ISO 12945-2

The specimen held in the fixture has a diameter of 140(0,+5) mm. Material placed on the pilling table may be circular with a diameter of 140(0,+5) mm or square with a side length of (150±2) mm.

Loose fibers or yarns around an edge can interfere with the friction area and cause wrinkling. Where needed, edges may be secured, for example by gluing or taping, to keep the test area in suitable condition.

A minimum of three specimen sets is required. Each set includes one specimen in the fixture and one specimen on the pilling table used as the abrasive. When a wool fabric abrasive is used on the pilling table, at least three specimens are tested. If more than three are used, the number selected should be odd. Additional specimens may also be prepared for comparative grading.

Role of a Martindale Abrasion and Pilling Tester

A Martindale abrasion and pilling tester is used with many textile structures to determine resistance to abrasion and pilling. During the evaluation, samples rub against a known abrading material at low pressure while the direction of movement changes continuously. The resulting surface condition is compared with the relevant grading references.

The source equipment description identifies a dual-servo-driven tester that produces a standard Lissajous motion trajectory. It also lists six selectable test modes: abrasion 60×60, pilling 24×24, 60-X, 60-Y, 24-X, and 24-Y. Selecting a mode can be done without hardware conversion according to the source information.

Visual Assessment and Pilling Grades

For grading, a 38 mm circular specimen is positioned squarely on double-sided adhesive tape in a rating box. Under suitable lighting, the front surface is compared with appropriate standard fabrics or photographs. The specimen is viewed from a 45° downward angle during assessment.

The reported grade describes the extent of surface abrasion and pilling observed:

GradeSurface condition
5No change.
4Slight surface abrasion and/or slight pilling.
3Moderate surface abrasion and/or pilling, with fiber balls of different sizes and densities covering part of the surface.
2Significant surface abrasion and/or pilling, with fiber balls of different sizes and densities covering most of the surface.
1Severe surface abrasion and/or pilling, with fiber balls of different sizes and densities covering the entire surface.

Using Results in Textile Quality Control

The ISO 12945-2 Martindale pilling test helps teams document how a fabric surface responds to rubbing and compare specimens evaluated under the same agreed conditions. It can support material evaluation during product development, incoming inspection, and quality-control activities.

A useful report should identify the specimen treatment condition, the number of specimens tested, the abrasive arrangement, and the visual grade assigned. Keeping these details together gives the grade its practical context and makes it easier to interpret differences between fabrics or production samples.

関連ニュース

What Is Fiber Polarity and How Do You Choose an MPO Method?
2026年11月14日 11時35分16秒

Fiber polarity ensures the transmit path connects to the corresponding receive path. For MPO-based duplex channels, the selected method must remain consistent across trunks, cassettes, adapters, and patch cords.

The scent of new wood in a newly handed-over apartment: How to measure and address formaldehyde (HCHO) levels before moving in
2026年11月14日 10時28分19秒

Many people refer to the pungent, acrid odor that emerges when opening a new cabinet as the "smell of new wood," assuming it will simply dissipate after a few days. In reality, however, what is being released could well be formaldehyde—a substance originating from the adhesives used in the pressed-wood panels—and our sense of smell is not a reliable enough gauge to determine the concentration levels present

Guide to Selecting a TCLP Toxicity Characteristic Leaching Procedure Shaker Configuration in Compliance with QCVN 07:2025/BNNMT and TCVN 9239:2012
2026年11月13日 17時23分39秒

Regulation QCVN 07:2025/BNNMT (replacing QCVN 07:2009/BTNMT and QCVN 50:2013/BTNMT) specifies hazardous waste and sludge thresholds based on leachate concentrations. To ensure that analytical results for heavy metals and organic compounds are accepted during ISO/IEC 17025 or VIMCERTS assessments, laboratories must comply with the Toxicity Characteristic Leaching Procedure (TCLP) specified in TCVN 9239:2012, which is equivalent to US EPA Method 1311

Checking the Temperature of Paint and Coating Surfaces After Curing Using an Infrared Thermometer
2026年11月13日 16時11分22秒

An infrared thermometer allows surface temperature measurement without direct contact, making it suitable for products coming out of curing ovens or surfaces that are difficult to access. However, to ensure reliable results for production quality control, it is important to understand the measurement principle and the factors that affect measurements on painted and coated surfaces.

Crowded Gyms and Yoga Studios: How to Manage Air Quality to Retain Members
2026年11月13日 15時07分40秒

Around 6 or 7 in the evening, the gym becomes packed; the music drowns out the sound of heavy breathing, and the air conditioning runs at full blast behind closed doors. At first glance, everything seems fine: the room is cool, the lights are bright, and the equipment is state-of-the-art. Yet, after just a few sessions, regular members begin to feel a heavy-headedness and find themselves running out of breath more quickly eventually, they simply stop renewing their memberships. No one complains about the personal trainers or the exercise machines. The very thing that makes them feel stifled and drives them away is something entirely invisible: the air inside the room

お得な情報を受け取る

数量割引、まとめ買い価格の更新、新製品情報をメールでお届けします。

登録することで、当社の利用規約およびプライバシーポリシーに同意したものとみなされます。

クイックサポート

認定専門家へ直接アクセス